Anionic polyacrylamide is sold on one headline number: molecular weight. Buyers compare 12 million against 18 million the way they compare AlβOβ content in PAC, as if higher is better. In a nickel tailings thickener, that assumption is wrong about as often as it is right.
Molecular weight controls the reach of the polymer chain. Charge density controls the grip. Bridging flocculation needs both, and the ratio between them has to match the particle size distribution of your slurry. A 20 million Da polymer in a coarse, fast-settling tailings will bridge across particles so long that the flocs trap water and the underflow density drops. An 8 million Da polymer in a clay slime will not reach across enough particles and the overflow stays turbid no matter how much you dose.
This article lays out a workable selection sequence for nickel operations, based on the two circuit types that dominate production today.
The two circuits behave nothing alike, and the polymer requirement follows the mineralogy rather than the brand of thickener.
| Parameter | HPAL laterite (limonite / saprolite) | Sulphide flotation tailings |
|---|---|---|
| Slurry pH before neutralisation | 1.0β2.5 (acid leach residue) | 8.0β10.5 (alkaline flotation) |
| Dominant solids | Iron oxide / hydroxide gel, silica, aluminium, magnesium | Serpentine, talc, pyrrhotite, quartz, ultramafic gangue |
| Particle character | Very fine, high surface area, gelatinous, slow to compact | Mixed, often coarse, but talc and serpentine create slime fractions |
| Typical polymer type | High charge anionic, sometimes amphoteric | Medium to high charge anionic |
| Typical molecular weight | 16β22 million Da | 8β16 million Da |
| Typical dose | 60β150 g/t dry solids | 15β60 g/t dry solids |
These are working ranges, not specifications. Every ore body sits somewhere inside them, and the only reliable way to pin down a number is a cylinder settling test on your own slurry.
Run a jar test sweep across charge densities (typically 10, 30, 50 and 70 mol% anionicity for nickel tailings) at a fixed, moderate molecular weight. Measure clarifier overflow turbidity and settling rate at 30 seconds, 1 minute and 5 minutes.
In laterite residue, the correct charge density is usually the highest one that does not overshoot into charge reversal. The signal for overshoot is a sudden rise in supernatant turbidity after passing through a clean minimum β the flocs have picked up a net negative charge and repel each other again. In sulphide tailings with significant talc, the picture is complicated by naturally hydrophobic slimes, and a moderate charge density with a lower molecular weight often outperforms the highest charge option.
This is where the practical answer emerges. Hold the charge density and vary molecular weight in four steps (for example 8, 12, 16 and 20 million Da). Record four numbers for each:
The results almost never point to the highest molecular weight. In coarse sulphide tailings, the lowest polymer that still clears the overflow is normally the most economical, because it delivers a drier underflow at a lower dose. In clay-heavy laterite residue, high molecular weight wins on settling rate but can lose on underflow density β a trade-off you have to price out, since underflow density sets your tailings dam water balance.
A high molecular weight floc is fragile by construction. Long chains mean long lever arms, and every pump impeller, static mixer and weir the floc passes through shortens it. Three practical rules:
A note on dosage units. Nickel operations often report polymer dose in g/t of dry solids, but the number that matters commercially is g/t of containing product. A 90% active powder at 60 g/t and a 35% emulsion at 60 g/t are not the same purchase. Always convert to active polymer before comparing quotes.
By the time a thickener underperforms, the conversation has usually moved to buying a higher molecular weight product. In our experience servicing nickel plants, roughly half of these cases are not a product problem at all β the polymer is being destroyed before it reaches the feedwell.
Anionic polyacrylamide loses molecular weight irreversibly under mechanical shear. The make-up tank agitator is the usual culprit. Practical limits:
| Stage | Recommended condition | What goes wrong |
|---|---|---|
| Make-up water temperature | 5β40 Β°C | Above 50 Β°C, hydrolysis accelerates and viscosity drops permanently |
| Powder wetting concentration | 0.1β0.3% active | Above 0.5%, "fish eyes" form and never dissolve |
| Agitator tip speed | Below 1.5 m/s (typically β€ 200 rpm on a 1 m impeller) | High shear cuts the chain; viscosity falls and dose climbs |
| Ageing / maturation time | 30β60 minutes before use | Under-matured solution underperforms by 20β30% |
| Solution storage life | Use within 24β48 hours | Beyond 3 days, biological and oxidative degradation begins |
Before ordering a higher molecular weight product, measure the viscosity of your working solution at the tank outlet and again at the feedwell. A drop of more than about 15% between the two points confirms mechanical degradation, and the fix is plumbing, not chemistry.
Molecular weight on a certificate of analysis is almost always a nominal figure derived from intrinsic viscosity, measured under laboratory conditions that bear no resemblance to your thickener. Ask instead for:
Hua Quan manufactures anionic, cationic, non-ionic and amphoteric polyacrylamide in powder and emulsion form, with molecular weight selectable across the 5β25 million Da range and anionicity adjustable between 10 and 70 mol%. For mining applications we supply industrial grade to GB/T 17514-2017, and we routinely run cylinder settling tests against customer tailings samples before quoting.
Because we operate six production sites and hold ISO 9001 and ISO 14001 certification, batch-to-batch consistency of intrinsic viscosity is controlled as a routine production parameter rather than a certificate formality. That matters more in a thickener than the headline number on the datasheet.
Send us 2β5 kg of your slurry with the operating pH, solids content and target underflow density. We will run a charge density and molecular weight sweep and report the recommended product with the settling data attached.
The dosage ranges and operating limits in this article are typical industry values for guidance only. Actual performance depends on ore mineralogy, water chemistry and circuit configuration. Always confirm by bench or pilot test on your own slurry before setting plant dosing.