Every supplier has a specification sheet with a molecular weight and a charge density on it. Those two numbers describe the product. They do not describe your tailings. The behaviour of a flocculant in a thickener depends on the particle size distribution of the solids, the clay fraction, the dissolved ion load, the pH, the temperature, and how much mechanical shear the floc will see between the dosing point and the underflow. None of that appears on a mineral assay.
This is why two deposits with essentially identical chemistry can behave differently. A laterite slurry with 30% clay-sized fines and a sulphide tailings with 5% fines will not respond to the same polymer, will not settle at the same rate, and will not produce the same underflow density — even if the assay table is indistinguishable. The product that works on one will underperform on the other, and the only way to find out is to run both on real slurry.
| Variable | Why the assay misses it | What it changes |
|---|---|---|
| Particle size distribution | Reported as a single P80 figure at best | Sets the required chain length; fines fraction dominates the polymer demand |
| Clay mineralogy | Rarely assayed | Smectite and illite carry high surface charge and consume polymer; kaolinite behaves differently again |
| Dissolved ions | Only major ions usually reported | High ionic strength screens the charge on the polymer and shortens its effective reach |
| Residual reagents | Not an ore property | Flotation collector, depressant and frother all compete for adsorption sites |
| Temperature | Seasonal, not geological | Slows kinetics and raises the required dose in winter |
| Shear history | Plant design, not the ore | Long chains are cut before they can bridge; the fix is plumbing, not chemistry |
The value of the test is not the recommended product. It is the dose-response curve, the underflow density, and the confidence that the number will hold at scale. A typical programme runs as follows.
What to record, beyond the numbers. Floc size and strength, the appearance of the supernatant, and how the mud line behaves in the first 30 seconds are as predictive as the turbidity figure. A large, strong floc that settles fast at 2 NTU is a better operating result than a fine, fragile floc at 1.5 NTU that breaks when the thickener rakes.
Plot supernatant turbidity or TSS against dose. The curve falls steeply, flattens, and then — in most slurries — rises again as you pass the optimum. The rise is charge reversal and restabilisation, and it is the most expensive thing that happens in flocculant selection, because the natural operator response is to add more polymer.
| Observation | What it means | What not to do |
|---|---|---|
| Turbidity falls then rises as dose increases | You have passed the charge-neutralisation optimum | Do not raise the dose — step back down |
| Settling rate good, supernatant still turbid | Wrong charge density; the flocs are trapping fines instead of capturing them | Do not switch to a higher molecular weight yet |
| Clear supernatant, slow settling | Chain length too short to bridge across the particle population | This is the case for a higher molecular weight |
| Bench good, plant poor | Shear in the plant, or the sample was not representative | Do not order a different polymer until the shear question is settled |
| Result varies between repeats | Sample heterogeneity, or the slurry is ageing | Do not draw a conclusion from one run |
Any supplier can quote a price per tonne. A supplier who intends for the product to work will provide, at minimum:
If a supplier quotes a single dose without running anything, that number is a guess. It may be an educated guess, but it will be your plant that pays to find out.
We supply polyacrylamide across the full 5–25 million Da range with anionicity adjustable between 10 and 70 mol%, in powder and emulsion form, to GB/T 17514-2017. But the specification is only useful if it matches the slurry, so our standard commercial process is: sample in, bench programme out, then a quotation that carries the settling data with it.
Our laboratory at Base 2 runs jar test stations, particle size analysis and full wet chemistry in house, which means the turn-round on a sample is measured in days rather than weeks. For mining projects we will also run the test on a second charge density and molecular weight combination once the first round is in, so the recommendation is a curve rather than a point.
ISO 9001 and ISO 14001 certification applies across all six production sites, and batch-to-batch intrinsic viscosity is controlled as a routine production parameter — which matters more in a thickener than the headline number on the datasheet.
Send 2–5 kg of representative slurry with the operating pH, solids content and target underflow density. We will run a charge density and molecular weight sweep and report the recommended product with the settling data attached — no obligation to purchase.
Dose ranges, settling rates and optimum conditions described in this article are illustrative of the test method rather than performance guarantees. Actual results depend on ore mineralogy, water chemistry, temperature and plant configuration. Bench results should always be confirmed by plant trial before full-scale changeover.